Fabric testing
- Bursting strength
- Crocking
- Fiber composition
- Light fastness
- Perspiration fastness
- pH value
- Pilling
- Shrinkage
- Spirality
Bursting strength: where the fabric gives way
Knits fail by bursting rather than by tearing. This test puts a number on the pressure a fabric survives.

What this test measures
The force required to rupture the fabric when it is pushed from one side.
How the test is run
1. The specimen is clamped over an expanding diaphragm without tension.
2. Pressure is applied at a controlled rate, expanding the diaphragm against the fabric.
3. The test ends at rupture; the peak pressure is recorded.
4. Several specimens are tested and the result reported as the mean.
How we report the result
Bursting strength in kPa, with the number of specimens tested stated alongside the mean - a mean without its sample count is not reproducible.
Why it matters to you
Elbows, knees and seat seams are where lightweight knits wear through. Bursting strength is the closest laboratory proxy for whether a fabric survives being stretched over a body, and it is the number to quote when a buyer compares two weights of the same article at the same price.
What causes a failure
- Lower GSM than the article was developed at.
- Coarser gauge or reduced stitch density at the same weight.
- Resin or finish that embrittles the yarn.
FAQ
Q: Does higher GSM always mean higher bursting strength?
A: Usually, but gauge and stitch density can override weight.
Q: Is this the same as tensile strength?
A: No - knits are better characterised by bursting than by strip tensile.
Crocking: does the color rub off?
Crocking is the test behind the complaint that a dark garment marked a white sofa, a bag strap or a wearer's skin.

What this test measures
How much color transfers from the fabric to another surface under rubbing, measured separately in dry and wet conditions.
How the test is run
1. The specimen is mounted flat on the crockmeter base.
2. A white crock cloth is rubbed against it with a 16 mm diameter finger under controlled load and stroke count.
3. The procedure is repeated with a wetted crock cloth for the wet result.
4. The staining on the crock cloth is rated against the AATCC Grey Scale.
How we report the result
Grey Scale 1–5 in half steps. Dry and wet are always reported as two separate figures - a single "crocking 4" hides which condition was tested, and wet is almost always the lower of the two.
What our fabrics achieve
Why it matters to you
Wet crocking is the first property to fail in summer weight and activewear, because perspiration and friction act together. For dark and saturated shades, this is the number to agree before bulk, not after the first complaint.
What causes a failure
- Insufficient soaping and rinsing after dyeing, leaving unfixed dye on the surface.
- Heavy shades dyed without a compatible after-treatment.
- Poor drying control, which brings dye back to the surface.
FAQ
Q: Which matters more, dry or wet?
A: For next-to-skin and activewear, wet.
Q: Can a failing lot be reworked?
A: Often yes, by re-washing and re-fixing, subject to shade matching.
Fiber composition: what the fabric is actually made of
A composition claim is only worth the test behind it. This page covers how we identify the fibers in a knit and how we measure their proportions.

What this test measures
Two separate questions. AATCC 20 identifies which fiber types are present. AATCC 20A determines how much of each one, by weight.
How the test is run
1. A representative sample is taken from the bulk lot, not from the development sample.
2. Fibers are identified by microscopy and by solubility behaviour in selected reagents (AATCC 20).
3. Each component is separated by chemical dissolution and weighed (AATCC 20A).
4. Percentages are calculated by dry weight and reported per declared fiber.
How we report the result
Percentage by weight for every fiber named on the spec sheet, to one decimal place, per batch. Where a blend contains elastane, the elastane content is reported separately because it is usually the number a buyer checks first.
What our fabrics achieve
Why it matters to you
This is the test behind the composition on your care label and on the customs declaration. If a mill cannot produce it per batch, the blend stated in the quotation is an assumption - and a labelling error becomes your liability, not theirs.
What causes a failure
- Sampling from the lab dip instead of the production lot.
- Elastane under-declared because it is hard to separate cleanly.
- Blended yarns where components cannot be fully separated by dissolution.
FAQ
Q: Is testing done per batch or once per article?
A: Per batch on request; per article during development.
Q: Can you test a fabric we did not buy from you?
A: Yes - composition testing works on any sample.
Light fastness: does the shade fade in sunlight?
Shop windows, hanging displays and daylight do more damage to some shades than washing ever will. This test isolates that exposure.

What this test measures
How much the color changes after a defined dose of artificial sunlight.
How the test is run
1. The specimen is mounted alongside a reference standard in the xenon-arc apparatus.
2. Under Option 3 the lamp runs on a continuous light cycle, without a dark period.
3. Exposure continues for a defined number of AATCC Fading Units (AFU) - we test at 20 AFU by default, with 40 AFU available on request.
4. The color change is rated against the Grey Scale.
How we report the result
Rating 1–5 with the exposure level in AFU stated next to it. A light fastness grade without its AFU figure cannot be compared with anything, because exposure is what produces the fade.
What our fabrics achieve
Why it matters to you
Bright and pale shades fail here before they fail anywhere else, and the failure is not reversible. If your product ships to markets with strong daylight or spends time in a window, this test determines the shelf life of the color.
What causes a failure
- Dye selection matched to shade rather than to end use.
- Light-sensitive shades - certain turquoise, violet and bright red ranges.
- Insufficient UV stabilisation in the finish for outdoor-adjacent use.
FAQ
Q: At what exposure do you test?
A: 20 AFU by default; 40 AFU on request. The level is stated with every rating.
Q: Does the fabric type affect the result?
A: Yes - mainly through dye uptake and fiber lustre.
Perspiration fastness: does color move against skin?
For anything worn next to the body, sweat is a harsher test than washing. This page covers how we measure that.

What this test measures
Whether the color changes, or transfers onto adjacent fabric, after contact with artificial perspiration.
How the test is run
1. Specimens are wetted out with artificial perspiration solution - one set acidic, one set alkaline.
2. Each specimen is placed in contact with a multi-fiber adjacent fabric.
3. The assembly is held under a specified load at elevated temperature for a defined period.
4. Both color change and staining are rated against the Grey Scale.
How we report the result
Four figures: color change and staining, each for acid and for alkaline. Collapsing these into one number loses the information that matters most - acid and alkaline results often differ by a full grade.
What our fabrics achieve
Why it matters to you
Underwear, activewear, loungewear and babywear are all judged on this. It is also one of the first documents a buyer's QA team requests, because a perspiration failure reaches the market as a returned garment rather than as a lab report.
What causes a failure
- Dye classes with poor wet-fastness used on deep shades.
- Incomplete reduction clearing on polyester and its blends.
- Softeners or finishes that migrate and carry dye with them.
FAQ
Q: Do you test both acid and alkaline?
A: Yes - always both.
Q: Does this replace wash fastness testing?
A: No; they stress the fabric differently and are reported separately.
pH value: what is left in the fabric
pH does not appear in a garment's marketing, but it appears in its returns. This page covers how we measure what processing leaves behind.

What this test measures
The acidity or alkalinity of the fabric's water extract - a proxy for residual chemicals left after dyeing and finishing.
How the test is run
1. A weighed specimen is immersed in distilled water.
2. The extraction is held at elevated temperature for a defined period.
3. The extract is cooled and its pH measured with a calibrated electrode.
4. The result is reported to one decimal place.
How we report the result
A single pH figure to one decimal place, per fabric and per batch. pH is a measurement, not a grade - it does not sit on the same 1–5 scale as the fastness tests, and we keep it separate for that reason.
What our fabrics achieve
Why it matters to you
Skin comfort and compliance for next-to-skin and baby products. Residual alkali from scouring and dyeing is invisible, does not affect hand feel much, and is one of the few defects that only a laboratory will catch before a customer does.
What causes a failure
- Insufficient rinsing after scouring or dyeing.
- Alkaline dyeing systems neutralised incompletely.
- Residues from some softeners and fixing agents.
FAQ
Q: What range is acceptable?
A: Set by your destination market and product type; we report the measured value and work to your limit.
Q: Does pH change over time in storage?
A: Little, if the fabric is stored dry and neutral.
Pilling: does the surface fuzz up?
Pilling is slow, visible and hard to reverse. This test reproduces in hours what a customer would see after a month of wear.

What this test measures
How much loose fibre migrates to the surface and forms pills under repeated abrasion.
How the test is run
1. Specimens are mounted on the Martindale instrument against an abradant.
2. The test runs for 2,000 rubs - the level we use for apparel knits; 7,000 rubs is available on request.
3. Specimens are assessed at the end of the run against the pilling photographic scale.
4. The result is recorded per specimen and reported as the common grade.
How we report the result
Pilling grade 1–5, where 5 is no pilling, together with the rub count. A grade without the rub count is not comparable, since pilling continues to develop with wear.
What our fabrics achieve
Why it matters to you
Pilling shows up first at cuffs, underarms and seat - the places a customer judges quality without being told to. On soft spun yarns it is the property most likely to trigger a complaint that no other test predicts.
What causes a failure
- Short-staple or loosely twisted yarn in the face of the fabric.
- Excessive surface brushing or raising in finishing.
- Blends where one component is weaker and migrates to the surface.
FAQ
Q: Which standard do you test to?
A: ISO 12945-2 (Martindale) at 2,000 rubs. ASTM D3512 is available on request for US specifications.
Q: Does washing make pilling worse?
A: It can, by loosening surface fibre; we assess both as-worn and after-laundering on request.
Shrinkage: how much the garment moves after washing
"Shrinkage 3%" tells you almost nothing. This page explains what we measure, in which direction, and under which laundering conditions.

What this test measures
The percentage change in length and in width after home laundering, measured against bench marks placed on the fabric before washing.
How the test is run
1. Bench marks are applied to the specimen at a fixed gauge length.
2. The specimen is laundered under the conditions of AATCC 135 Option 1 - wash cycle, temperature, detergent and drying procedure are fixed by that option.
3. The specimen is conditioned and re-measured at the same gauge points.
4. Change is calculated separately for length and width.
How we report the result
Two figures - length and width - as percentage change, with the wash temperature, cycle and drying method stated. Without those three conditions the number cannot be reproduced in another lab, which is why we publish them together.
What our fabrics achieve
Length :2%-5%
Width:1%-3%
Why it matters to you
This predicts whether the finished garment still fits after the first wash - the most common reason a first order becomes a repeat order, or does not. Length and width move in different directions on knits, so a single combined figure will mislead your pattern team.
What causes a failure
- Insufficient relaxation before cutting, so shrinkage appears after the customer washes it.
- Tension built into the fabric during finishing and winding.
- Heat setting skipped or under-run on elastane blends.
FAQ
Q: Is shrinkage measured before or after finishing?
A: On finished, relaxed fabric - what the cutter actually receives.
Q: Can you supply fabric pre-relaxed to a tighter tolerance?
A: Yes, within limits; the tighter tolerance affects lead time.
Spirality: does the panel twist after washing?
A leg that spirals after the first wash is one of the most expensive failures to correct, because the fabric is already cut. This test finds it earlier.

What this test measures
How far a square of fabric deforms from a right angle after home laundering - the same mechanism that makes a finished leg twist.
How the test is run
1. A square specimen is marked with reference lines before laundering.
2. The specimen is laundered and dried under the specified conditions.
3. The displacement of the reference marks is measured after conditioning.
4. Skew is expressed as a percentage of the original dimension.
How we report the result
Skew percentage after laundering, with the number of wash cycles and the laundering conditions stated. We test after the cycle count agreed with the buyer, typically after three home launderings.
What our fabrics achieve
Why it matters to you
Spirality is a fabric property that becomes a garment defect. It depends on yarn twist direction, machine rotation and relaxation, so it cannot be corrected at cutting once the bulk is woven - it has to be controlled during knitting and finishing.
What causes a failure
- High twist in the yarn combined with insufficient relaxation.
- Single jersey structures with more feeds per diameter.
- Tubular fabric slit without allowing for the natural skew direction.
FAQ
Q: When is spirality measured?
A: After laundering - the deformation only appears once the fabric relaxes in water.
Q: Can a high-skew lot be used?
A: Sometimes, by cutting on the skew, but this consumes more fabric and limits panel shapes.